[1103] DETERIORATION OF CONCRETES CONTAINING SHIRASU NATURAL POZZOLAN AND LIMESTONE POWDER EXPOSED TO AGGRESSIVE CHEMICAL ENVIRONMENT

Van Toan PHAM1, Meng PHALKONG1, 小川由布子2, 河合研至2 (1.Hiroshima University, 2.広島大学)

キーワード:compressive strength、deterioration of concrete、limestone powder、magnesium chloride、Shirasu、sulfuric acid

This study investigated the deterioration of concretes caused by the attack of an aggressive chemical solution composed of 3% sulfuric acid and 5% magnesium chloride. A part of fine aggregate was replaced with Shirasu natural pozzolan and/or limestone powder. The results showed that after 12 weeks of immersion, the compressive strength loss, neutralization depth and chloride penetration depth of concrete containing Shirasu were lower than those of concrete without Shirasu. The addition of limestone powder can result in more severe deterioration of concrete.