9:30 AM - 9:45 AM
[10a-Z03-3] Deposition of tungsten nitride films by thermal CVD using liquid source material
Keywords:tungsten nitride, thermal CVD, hexamethyldisilazane
Generally, tungsten nitride (W2N) films are deposited by using PVD or thermal CVD with the use of WF6, NH3 and SiH4. But there are step coverage issues when using PVD, and problems with safety and high cost with the use of NH3 or SiH4 when using thermal CVD. In this study, we tried to deposit W2N films by thermal CVD using WF6 and 1,1,1,3,3,3-hexamethyldisilazane, which is a non-explosive, inexpensive and liquid with Si-N bonds. X-Ray diffraction pattern showed W2N (111) and (200) diffraction peaks. In addition, cross-section SEM image showed excellent step coverage of the deposited W2N on trench pattern with an aspect ratio of 7.